Powder Coating Common Problem Solution - The Film Flow Leveling Is Not Good From The Formula How To Solve
Coating industry: Problem: After the construction of powder coating film are peel brush marks, corrugated, shrinkage and other irregular shape. Affect the surface of the decorative and beautiful, how to solve the problem from the adjustment formula. Answer: Taking into account the storage stability of the powder coating, the use of resin glass temperature, high softening point, high melting viscosity of the resin, so that the high melting viscosity of powder coatings, film leveling is not good, there is a choice of pigment and filler oil absorption is higher, so that the powder coating melt viscosity increased, film leveling is not good. Specific solutions are: (1) select the low melt viscosity of polyester resin, the epoxy resin to choose a little lower softening point varieties. (2) Select the appropriate amount of pigment, try not to use too much, especially the large amount of oil absorption of organic pigments and carbo...